Three ways rubber gets into asphalt
The Federal Highway Administration's 2020 report Resource Responsible Use of Recycled Tire Rubber in Asphalt Pavements (FHWA-HIF-20-043) groups today's technologies into three families. Each one buys crumb rubber differently.
| Process | Where rubber is added | Typical GTR size (FHWA) | Typical GTR dosage (FHWA) |
|---|---|---|---|
| Wet process, asphalt rubber (AR) | Blended into hot binder at or near the plant, reacted 30-60 min | Max around 1.5 mm (15 mesh) | 10-22% by weight of binder |
| Terminal blend (RMB) | Blended at a fixed terminal, stored hot, shipped like regular binder | 30-80 mesh; 30-40 mesh most typical ("30 minus rubber") | 5-15% by weight of binder |
| Dry process | Added to the mix through the RAP collar | 30-40 mesh | ~10% by weight of binder ≈ 0.5% of mix ≈ 10 lb per ton |
FHWA also notes the wet-process portable blending plants receive GTR "in bulk or super-sacks." That's exactly how we ship.

What "asphalt rubber" means, officially
ASTM's definition (in ASTM D8 terminology, with physical requirements in ASTM D6114, Standard Specification for Asphalt-Rubber Binder) is:
"A blend of asphalt cement, reclaimed tire rubber, and certain additives in which the rubber component is at least 15 percent by weight of the total blend and has reacted in the hot asphalt cement sufficiently to cause swelling of the rubber particles."
FHWA's 2023 TOPS how-to guide adds that blends with less than 15 percent rubber "are generally called rubberized asphalt or sometimes rubber modified asphalt." So the words matter: if a spec says asphalt rubber, it means 15%+ rubber, wet process.
State specs that drive demand
California (Caltrans)
Caltrans is the heaviest user of asphalt rubber in the country. Per the Caltrans Construction Manual (Section 4-39), asphalt rubber for rubberized hot mix asphalt (RHMA) includes 18 to 22 percent crumb rubber modifier (CRM) by total mass of the asphalt rubber blend, and the CRM must include 25 percent ± 2 percent high natural rubber content. Caltrans also requires extender oil. FHWA's TOPS guide reports that, as of 2023, asphalt-rubber gap-graded mixtures made up approximately 35 percent of Caltrans' annual tonnage placed.
Caltrans' CRM requirements live in Standard Specifications Sections 37-2.04, 39-2.03 and 92-1.02B, and Caltrans Test Method CT 385 covers CRM sampling and testing.
Arizona (ADOT)
ADOT Section 1009 governs asphalt-rubber material. As reproduced in a 2012 international specification summary, it requires:
- Minimum 20 percent ground rubber by weight of the asphalt cement
- Rubber specific gravity of 1.15 ± 0.05
- Free of wire; fabric no more than 0.1% (Type A) or 0.5% (Type B)
- Up to 4% calcium carbonate allowed to keep particles from sticking
- Certificates that the rubber came from whole scrap tires or shredded tire material from vehicles operated in the U.S.
ADOT's gradation bands have been revised over the years, so always pull the current book. We'll check our lot against whichever edition your contract cites.
The Midwest
FHWA's report lists dry-process projects built since 2007 in states including Illinois, Indiana and Wisconsin, and notes "dry-mix" projects placed in Michigan and Ohio. Shipping from Central Ohio, we're a short haul to all of them.
Worked examples
Example 1: Wet-process AR, Arizona-style
ADOT's minimum is 20 lb of rubber per 100 lb of asphalt cement. For every 100 tons of asphalt cement:
- Rubber = 100 × 20% = 20 tons = 40,000 lb
- That's about one full truckload (roughly 20 supersacks)
- Note: 20 parts rubber in 120 parts total is about 16.7% of the blend, comfortably over ASTM's 15% threshold for "asphalt rubber"
Example 2: Caltrans RHMA binder
For 100 tons of asphalt-rubber binder at 20% CRM (inside Caltrans' 18-22% band):
- Total CRM = 20 tons
- High natural CRM at 25% of CRM = 5 tons
- Scrap tire CRM at 75% = 15 tons = 30,000 lb
The high-natural portion has its own requirements; our scrap tire crumb covers the 75% side.
Example 3: Dry process in the Midwest
A 50,000-ton overlay using a dry-process additive at FHWA's rule of thumb of ~10 lb GTR per ton of mix:
- 50,000 × 10 lb = 500,000 lb of 30-40 mesh
- About 250 supersacks, or 12 to 13 truckloads, which we can cover from 30-minus inventory
Your additive supplier and mix design set the dose. We set the delivery schedule.
Bidding a rubber job? Get crumb priced to the plant. Send grade, volume, delivery city/ZIP and your target price.
Request a QuoteWhich of our grades fit
- 30-minus: in stock by the millions of pounds. FHWA calls 30-40 mesh "30 minus rubber" in terminal blends; dry processes use 30-40 mesh.
- 40 mesh and 80 mesh: made to order for faster-reacting binders.
- 20-30 and 10-20: coarser, for wet-process gradations that call for them. FHWA puts the wet-process typical max at about 1.5 mm.
Every one ships in supersacks, with or without pallets, with lot sieve data on request.
Frequently asked questions
What is the difference between asphalt rubber and rubberized asphalt?
By ASTM's definition, asphalt rubber has at least 15% rubber by weight of the blend and is reacted in hot asphalt (wet process). Lower-rubber blends are generally called rubberized or rubber-modified asphalt.
What mesh crumb rubber is used in asphalt?
FHWA reports typical paving GTR from about 1.5 mm down to 420 µm (15 to 40 mesh), with limited use of 80 and 120 mesh. Terminal blends most often use 30-40 mesh; dry processes use 30-40 mesh.
How much rubber goes into a ton of dry-process mix?
FHWA's rule of thumb is about 10 lb of GTR per ton of mixture (about 10% by weight of binder, roughly 0.5% of the mix).
Does your crumb meet Caltrans or ADOT specs?
We check each lot against the spec section you send. We don't claim agency compliance until it's documented for that lot.
Do you ship to asphalt plants and terminals?
Yes. Supersacks to the plant, or the terminal, on your schedule. FOB Central Ohio or delivered.
Sources: FHWA, FHWA-HIF-20-043 (2020) (PDF); FHWA TOPS Asphalt Rubber Gap-Graded Mixtures How-To (PDF); ASTM D8 and D6114; Caltrans Construction Manual §4-39 (dot.ca.gov); Caltrans CRM list (mets.dot.ca.gov); ADOT §1009 as reproduced in Summary of Rubber Modified Asphalt Product Specifications around the World (2012) (PDF).