Asphalt Rubber Specs, Decoded

If you bid rubber jobs or supply the crumb for them, three documents run your life: ASTM's definition and D6114, the Caltrans book, and ADOT Section 1009. Here's what each one actually requires of the rubber.

Asphalt-rubber blending unit fed by a crumb rubber supersack

Start with the words: asphalt rubber vs. rubberized asphalt

Half the confusion in this business is vocabulary. ASTM's definition, in its D8 terminology standard and used with the D6114 binder specification, is the anchor:

Asphalt rubber is "a blend of asphalt cement, reclaimed tire rubber, and certain additives in which the rubber component is at least 15 percent by weight of the total blend and has reacted in the hot asphalt cement sufficiently to cause swelling of the rubber particles."

Two requirements hide in that sentence:

  1. At least 15% rubber by weight of the total blend.
  2. Reacted. The rubber has to swell in hot asphalt, which is why asphalt rubber is a wet process.

FHWA's 2023 TOPS how-to guide adds the flip side: blends with less than 15 percent reclaimed tire rubber "are generally called rubberized asphalt or sometimes rubber modified asphalt." So when a spec says "asphalt rubber," you're in 15%-plus territory. When it says "rubberized" or "rubber-modified," read further.

ASTM D6114: the binder spec

ASTM D6114, Standard Specification for Asphalt-Rubber Binder, sets physical property ranges for the finished binder. FHWA's TOPS guide notes many state DOTs require asphalt rubber to meet D6114's physical requirements and then add their own: base binder grade, percent GTR, reaction time and temperature, and end-result properties. Common tests include rotational viscosity, resilience, softening point and cone penetration.

D6114 groups binders into three types by climate: Type I for hot climates, Type II for moderate and Type III for cold, as suggested guidelines tied to average monthly temperatures. Massachusetts, for example, calls for D6114 Type II in its crumb-rubber-modified asphalt spec, per FHWA's TOPS document.

What D6114 means for the crumb supplier: the rubber has to produce a binder that hits those properties with the contractor's asphalt and process. Gradation, source and cleanliness all affect that, which is why the agency specs below get so specific about the rubber.

Asphalt-rubber blending unit fed by a crumb rubber supersack
Wet-process blending: crumb from supersacks into hot asphalt, reacted before mixing.

Caltrans: the biggest asphalt-rubber program

California uses more asphalt rubber than anyone. FHWA's TOPS guide reports that as of 2023, asphalt-rubber gap-graded mixtures made up approximately 35 percent of Caltrans' annual tonnage placed.

The Caltrans Construction Manual (Section 4-39) summarizes the rubber requirements for rubberized hot mix asphalt (RHMA):

  • Asphalt rubber includes 18 to 22 percent crumb rubber modifier (CRM) by total mass of the asphalt rubber blend
  • The CRM must include 25 percent ± 2 percent high natural rubber content scrap rubber by mass of the CRM, which may come from scrap tires or other sources
  • Extender oil is required as an asphalt modifier
  • RHMA includes gap-graded (RHMA-G), open-graded friction course (RHMA-O) and open-graded high binder (RHMA-O-HB)

Caltrans lists two CRM material specifications, scrap tire crumb rubber and high natural scrap tire crumb rubber, with requirements in Standard Specifications Sections 37-2.04A(4)(C)(iii), 39-2.03A(4)(e)(ii)(C) and 92-1.02B. Caltrans Test Method CT 385 covers sampling and physical testing of CRM. Caltrans also maintains an Authorized Material List for CRM.

The Rubberized Asphalt Foundation's usage guide describes high natural rubber as a scrap rubber product with 40-48 percent natural rubber or isoprene and a minimum of 50 percent rubber hydrocarbon under Caltrans requirements, from sources including some heavy truck tires, tennis balls and mat rubber.

Caltrans math

100 tons of asphalt-rubber binder at 20% CRM

  • CRM = 20 tons
  • High natural CRM (25%) = 5 tons
  • Scrap tire CRM (75%) = 15 tons = 30,000 lb

At a typical 2,000 lb supersack, the scrap tire portion is about 15 sacks. That's under one truckload for 100 tons of binder.

Arizona: ADOT Section 1009

Arizona pioneered asphalt rubber. FHWA recounts ADOT's research in the mid-1970s and its adoption of GTR in interlayers, chip seals, and later open- and gap-graded mixes.

ADOT Section 1009, Asphalt-Rubber Material, as reproduced in a 2012 international specification summary, includes these rubber requirements:

  • Minimum 20 percent ground rubber by the weight of the asphalt cement
  • Gradation per Arizona Test Method 714, with Type A and Type B bands (ADOT has used Type B for hot mix)
  • Specific gravity 1.15 ± 0.05
  • Free of wire; fabric no more than 0.1% (Type A) or 0.5% (Type B)
  • Up to 4% calcium carbonate by weight of the rubber allowed to prevent sticking
  • Certificates confirming the crumb comes from whole scrap tires or shredded tire materials from vehicles owned and operated in the U.S., and that processing doesn't leave water-holding casings as waste
  • Asphalt cement is a PG binder; ADOT has used different base grades for desert, mid-zone and alpine climates

An asphalt-rubber presentation hosted by Arizona State University's pavement engineering program shows a later ADOT table with a revised Type B band, which is a good reminder: gradation bands change between editions. Pull the edition your contract cites.

"20% by weight of asphalt" is not 20% of the blend

This trips people up. ADOT's minimum is 20 lb of rubber per 100 lb of asphalt cement. In the blend, that's 20 ÷ 120 = 16.7% rubber, still over ASTM's 15% line. An ADOT training slide uses 23.5 lb of rubber per 100 lb of asphalt cement as an example and notes that equals about 19% by weight of the binder.

ADOT math: 500 tons of asphalt cement

  • Minimum rubber = 500 × 20% = 100 tons = 200,000 lb
  • About 100 supersacks, or 5 truckloads
  • At 23.5 lb per 100 lb (a common design level), rubber = 117.5 tons = 235,000 lb, about 6 loads

How FHWA frames the three processes

FHWA's 2020 report (FHWA-HIF-20-043) puts the agency specs in context:

Process GTR dose Typical GTR size
Wet process (AR) 10-22% by weight of binder Max around 1.5 mm (15 mesh)
Terminal blend (RMB) 5-15% by weight of binder 30-80 mesh; 30-40 most typical, "30 minus rubber"
Dry process ~10% by weight of binder (~0.5% of mix, ~10 lb per ton) 30-40 mesh

FHWA notes AR processing at about 350-375°F with 30 to 60 minutes of reaction before the binder goes into the mix, and that GTR typically arrives at the plant "in bulk or super-sacks."

What the crumb supplier should hand you

For any agency asphalt-rubber job, ask your crumb supplier for:

  1. Gradation by the agency's test method (ATM 714 for ADOT; CT 385 for Caltrans) or ASTM D5644 where allowed
  2. Fabric/fiber and wire/metal results against the spec limits
  3. Specific gravity, if required
  4. Source certification: whole scrap tires, U.S.-origin vehicles, as required
  5. Moisture, because water foams hot asphalt
  6. Parting agent content, if used
  7. Authorized material list status where the agency maintains one

We'll check any lot against the spec section you send. We don't claim agency compliance until it's documented for that lot.

Midwest buyers: where this applies to you

Midwest DOTs lean more on terminal blends and dry processes than on Arizona-style wet process. FHWA lists dry-process projects in Illinois, Indiana and Wisconsin since 2007, and dry-mix projects in Michigan and Ohio. The same principles apply: know the dose, know the gradation band, demand lot data.

Our 30-minus sits right in FHWA's "30 minus rubber" sweet spot for terminal blends and dry processes, and it's in stock by the millions of pounds in Central Ohio.

Bidding a rubber job? Get crumb priced to the plant. Send grade, volume, delivery city/ZIP and your target price.

Request a Quote

A sample submittal package

When an agency or prime contractor asks for crumb rubber documentation, a clean package saves days. Here's what we put together for asphalt-rubber and rubber-modified work, and what you should expect from any supplier:

  1. Product data sheet naming the grade, the gradation band and the test method (ASTM D5644 for the sieve analysis unless the agency names its own method, such as Caltrans CT 385 or ADOT's ATM 714).
  2. Lot sieve report for the material actually shipping, not a typical from last year.
  3. Physical properties the spec calls out: specific gravity, moisture, residual steel, fiber content and, where allowed, the mineral filler (calcium carbonate or talc) added to keep the rubber free-flowing.
  4. Source certification, for example ADOT's requirement that the rubber come from U.S.-origin scrap tires.
  5. Shipping documents that tie the bill of lading to the lot number so QC can trace every sack.

If the spec calls for a blend of scrap tire rubber and high natural rubber, as Caltrans does, the package also needs the hi-nat component's data, and the blend ratio has to be documented.

Common mistakes that cost bids

  • Quoting the wrong gradation. "30 mesh" in one state is not the same band as in another. Always quote against the band in the special provision.
  • Ignoring the fiber limit. ADOT's Type A limit is 0.1% fabric. Fiber balls also clog metering equipment on the plant side.
  • Forgetting the extender oil and hi-nat. In Caltrans asphalt rubber the binder supplier and the rubber supplier both have to be lined up before bid day.
  • Moisture. Wet crumb foams in hot binder. Keep sacks covered at the plant and check moisture on arrival.
  • Assuming one lot covers the job. Long jobs pull from several lots. Ask for each lot's sieve report as it ships.

Bringing it back to the Midwest

Most of the formal asphalt-rubber specifications discussed here come from the West and South, where the wet process grew up. In Ohio, Michigan, Indiana and their neighbors, ground tire rubber shows up more often as terminal-blend binder or dry-process mix (FHWA lists dry-process projects in Illinois, Indiana, Missouri and Wisconsin and dry-mix work in Michigan and Ohio). The same principles apply either way: know the gradation band, know the dose, and get lot data. A supplier who can read an Arizona or California spec can read a Midwest special provision too.

Frequently asked questions

What percentage of rubber is in asphalt rubber?

At least 15% by weight of the total blend under ASTM's definition. Caltrans specifies 18-22% CRM by total mass; ADOT requires at least 20% rubber by weight of the asphalt cement.

What is ASTM D6114?

The standard specification for asphalt-rubber binder physical properties.

What is high natural rubber CRM?

A scrap rubber product with high natural rubber content, required by Caltrans at 25% ± 2% of the CRM.

Is rubberized asphalt the same as asphalt rubber?

Not quite. Blends under 15% rubber are generally called rubberized or rubber-modified asphalt.

What crumb rubber size does ADOT use?

ADOT's Section 1009 has Type A and Type B gradations tested by ATM 714, revised over time. Check your contract's edition.

Sources: FHWA TOPS Asphalt Rubber Gap-Graded Mixtures How-To (PDF); FHWA-HIF-20-043 (2020) (PDF); Caltrans Construction Manual §4-39 (dot.ca.gov); Caltrans CRM Authorized Material List (mets.dot.ca.gov); Caltrans CT 385 (Jul. 2022); Rubberized Asphalt Foundation, Asphalt Rubber Usage Guide; ADOT §1009 as reproduced in Summary of Rubber Modified Asphalt Product Specifications around the World (2012) (PDF); J. Kliewer, Asphalt Rubber presentation (pavement.engineering.asu.edu); ADOT asphalt-rubber specifications training slides.

Need crumb rubber
by the truckload?

Send your grade, quantity and delivery ZIP or export destination. We'll review availability, packaging and freight, then come back with a written quote.

Request a Quote CallEmail